Acrylic roof coating is a water-based acrylic latex that dries as its water evaporates, leaving an elastic film over an existing roof. It is low in VOC and cleans up with soap and water, and white acrylics keep much of their reflectance. Its makers say it isn't for ponding water, and it needs mild, dry weather to go on.

ASTM standard
D6083, Type I or Type II
How it cures
Water evaporates; it dries rather than reacts
Volume solids
About 51 to 55%
Weather to apply
Usually 50°F or warmer, dry for hours after
Ponding water
Not for ponding water, its makers say
Warranty available
Up to 20 years from some makers, by thickness

What acrylic roof coating is

Acrylic roof coating is a water-borne emulsion of acrylic polymer. It cures by drying: the water evaporates out of the film, so cool or humid weather slows it down. Makers list VOC content under 50 grams per liter and soap-and-water cleanup, and the pails must not freeze.

About half of what goes on is water. Volume solids on makers' data sheets run about 51 to 55%, so a coat of 1.5 gallons per 100 sq ft goes on 24 mils wet and leaves about 12 mils dry. Gaco caps each coat at 1.5 gallons per 100 sq ft, so a thicker system means more coats.

A cured acrylic film lets water vapor through. A 2001 paper in IIBEC's journal calls waterborne acrylics inherent breathers, above 1.0 perm, and makers' data sheets list 7 and 25 perms.

ASTM D6083 is the standard specification for acrylic roof coatings: water-dispersed acrylic latex coatings applied by brush, squeegee, roller or spray. Like the other coating standards, it gives no guidance on application. Data sheets that print its requirements list a minimum of 200 psi tensile strength and 100% elongation.

D6083 has two types. BASF, whose staff led the change, says a 2018 revision kept the original as Type I and added Type II as an alternative that runs the low-temperature flexibility test at -10°C instead of -26°C. BASF says the colder test pushed makers toward soft polymers, which get tacky and pick up dirt. Sika and Karnak label their acrylics Type I, and Polyglass says its PG 700 meets both.

Pros and cons

Where acrylic coatings work

  • Water-based: under 50 g/L of VOC on makers' data sheets, and tools clean up with soap and water.
  • White acrylics keep much of their reflectance: Tremco's Solargard 6083 is rated 0.81 after three years outdoors and Karnak's 501 0.77.
  • The cured film breathes, letting water vapor out of the roof.
  • It can be recoated with more acrylic, or with silicone later.
  • With fabric embedded across the roof, it builds a thicker membrane, with warranties up to 20 years from Henry.

Where they fall short

  • Not for ponding water, its makers say, and some warranties exclude areas that hold water.
  • Weather-limited: usually 50°F or warmer, no freezing within 24 hours, dry for 4 to 48 hours after, and humidity under about 85%.
  • About half of it is water, so reaching a dry thickness takes about twice the wet mils and several coats.
  • Reflectance drops if the roof isn't cleaned regularly.
  • It can't go over silicone.

How it's applied

  1. Find wet insulation first. Henry says not to coat over saturated insulation and lists infrared scans among survey methods, Sika makes the applicator responsible for a moisture scan, and Karnak says not to coat a roof that is 20% or more wet.
  2. Wash the roof, usually at 2,000 psi or more, and treat algae and mildew with a bleach solution. Gaco is an exception on asphalt roofs: it says not to wash them except to remove biological growth.
  3. Test adhesion. Henry requires at least two tests, one per 10,000 sq ft, each at 2.0 pounds per inch or better to be eligible for its warranty.
  4. Repair seams, cracks and blisters with a three-course detail: sealant or coating, polyester fabric embedded in it, then more coating.
  5. Prime for the roof underneath: a rust-inhibitive primer on rusted metal, a bleed-blocking primer or base coat over asphalt so it doesn't yellow the white top coat, and separate primers for TPO and PVC and for EPDM.
  6. Apply a base coat, then the top coat across it, with an extra coat at edges and penetrations. Gaco lists 4 to 6 hours to dry between coats at 75°F and 50% humidity, and Tremco waits at least 24 hours.
  7. Allow for texture: rough and granulated surfaces take more coating to reach the same dry thickness, and Tremco adds 15 to 25% for ribbed metal panels.

Weather limits

Most acrylic data sheets set a 50°F minimum air and surface temperature, and Tremco wants temperatures rising after application. Some products allow 40°F: Karnak's 501 at 40°F and rising, and Gaco's 127.

Don't apply it when the dew point is within 5°F, or when temperatures could fall below freezing within 24 hours.

How long a fresh coat has to stay dry varies by product: Gaco's A47 4 hours (6 to 8 in high humidity), Henry 12 hours, Karnak 24 hours and Sika 48. Rain or dew before the film forms can wash it off or blister it, so makers say to coat in the morning; American WeatherStar says not within two hours of sunset.

Humidity has a ceiling too: Polyglass says not to apply above 84% relative humidity, and Karnak's spec allows the base coat at 85% or less.

In heat, Gaco allows a light water mist when the roof is over 100°F, Karnak recommends thin coats above 90°F, and Sika says to apply the base coat as temperatures fall.

Ponding water

Acrylic makers say their coatings aren't for ponding water. Gaco says its A47 isn't intended for surfaces prone to ponding and points buyers to its silicones when long-term ponding resistance is needed. Sika says its 515 AC isn't for ponding beyond 72 hours, and Tremco rules out continuous immersion.

So makers require positive drainage first, and some say to reslope or add drains. Karnak's data sheet gives the test it attributes to NRCA: no standing water 48 hours after rain stops. Progressive Materials uses 24 hours, and its specs exclude from the warranty any area that holds standing water after the work.

The 2001 IIBEC paper explains why: for an acrylic, the ponding question is really one of wet adhesion, because the more the film swells, the more it strains its bond to the roof.

ICC Evaluation Service reports for acrylic systems over spray foam and existing roofs require a slope of at least 1/4 inch per foot. Gaco's acrylic documents say they're not intended for slopes under 2:12.

Reflectance and dirt

Cool Roof Rating Council ratings for white acrylics, new and after three years outdoors: Tremco's Solargard 6083 white 0.85 and 0.81, Karnak's 501 Elasto-Brite 0.86 and 0.77, Henry's AcryShield A500 0.83 and 0.73, and Sika's Sikalastic 515 AC 0.83 and 0.69.

Texture and color matter. Polyglass's PG 700 is rated 0.75 after three years on a smooth surface and 0.67 on a rough one, and Gaco's A47 reflects 0.19 of sunlight in gray and 0.45 in tan, against 0.85 in white.

Makers advertise dirt pickup resistance, and American WeatherStar warns that reflectance drops if the roof isn't cleaned on a regular schedule.

Fabric-reinforced systems and foot traffic

Some acrylic systems embed polyester fabric across the whole roof, not just at seams, making a thicker fluid-applied membrane. Henry says the fabric adds about 8 to 13 mils, and American WeatherStar counts 15. Miami-Dade notes that fabric in a maintenance coating protects the roof underneath but doesn't make the coating a roof system.

Areas with regular foot traffic need protection. Sika recommends walkway pads, and Henry broadcasts granules into the wet coating at 20 to 30 pounds per 100 sq ft.

Recoating

Acrylic can go over an existing acrylic coating once it's identified and cleaned. Gaco's recoat spec calls for a power wash above 3,000 psi, a bleach solution on algae or mildew, and a fully dry roof.

Acrylic doesn't go over silicone: Gaco says not to apply its A47 over existing silicone, and Tremco lists silicone-based products among surfaces it doesn't recommend. Silicone can go over acrylic; Polyglass lists well-adhered acrylic coatings as a surface for its silicones.

Warranties and thickness

System warranties need a manufacturer-licensed applicator, and some makers approve or inspect the job before it starts and after it's done.

Thin spots aren't covered. Gaco says work that misses the minimum dry thickness isn't eligible for its labor-and-material warranty and suggests adding 10% to the coating ordered. It also excludes areas left untreated under equipment that wasn't lifted.

A product warranty is much narrower: Sika's data sheet warrants its 515 AC for one year against manufacturing defects, with the remedy limited to the purchase price or replacement product, not labor.

Makers set the term by total dry thickness:

  • Henry acrylic restoration: 26, 30 and 43 dry mils for 10, 15 and 20 years (32, 34 and 47 over granulated cap sheets).
  • Henry fabric-reinforced membrane: 38, 51 and 59 dry mils for 10, 15 and 20 years (49, 60 and 68 over granulated cap sheets).
  • Sika 515 AC: 26 dry mils for 10 years, 34 for 15, and 39 for 20 on metal roofs only.
  • Progressive Materials: 25 dry mils for 10 years over modified bitumen and built-up roofs; over metal, 22 for 10 years and 30 for 15.
  • American WeatherStar, fabric-reinforced over EPDM: 45, 50 and 58 mils for 10, 15 and 20 years, counting the fabric.
  • Gaco: up to 10 years on its A47 depending on thickness, and 5 years for a 12-mil recoat of an existing acrylic system.

Fire ratings

Fire classes under UL 790 (ASTM E108) belong to the whole roof assembly. ICC Evaluation Service reports on two fabric-reinforced acrylic systems over existing built-up roofs say the coated roof keeps the existing roof's class, whether A, B or C.

Over spray foam, Polyglass's report lists its acrylic-coated systems as classified roof coverings, each limited to a deck type and slope: for example, Class A over noncombustible decks up to 1:12 for one system and 2:12 for another. Miami-Dade's acceptance of an acrylic coating doesn't include a fire rating.

Other coatings

Roof systems

Calculator

Back to all roof coatings

Sources

  1. ASTM International, ASTM D6083/D6083M-24, Standard Specification for Liquid-Applied Acrylic Coating Used in Roofing
  2. Polyglass U.S.A., Inc., Technical Bulletin #2018-08: Guidelines for Applying Acrylics in High Humidity (Rev 013025)
  3. Gaco (Amrize Building Envelope), Product Data Sheet (PDS): GacoFlex A47 Series Acrylic Roof Coating (Revised 12/2022)
  4. Cool Roof Rating Council, Rated Products Directory: Tremco Solargard 1120 White, 0612-0012
  5. Cool Roof Rating Council, Rated Products Directory: Karnak 501 Elasto-Brite White, 0696-0003
  6. Sika Corporation, Product Data Sheet: Sikalastic-515 AC Acrylic Roof Coating (November 2025)
  7. BASF (acrylic resin maker), Q&A: Understanding the new ASTM Type-II standard for acrylic roof coatings (January 23, 2019)
  8. Polyglass U.S.A., Inc., Liquid-Applied Roof Solutions: Acrylic & Silicone Coatings, Primers & Accessories (brochure, 04/2026)
  9. Karnak Corporation, 501 Elasto-Brite product data sheet (01/11/21)
  10. American WeatherStar, Application Guideline: Acrylic Coating System with Polyester Fabric over EPDM
  11. Tremco Roofing and Building Maintenance, Solargard 6083 Base Coat data sheet
  12. Henry Company, Acrylic Restoration & Fluid Applied Membrane Systems Application Guide (04/24)
  13. Gaco (Amrize Building Envelope), Application Specification ASP-129-24-10: GacoFlex 129 Series Acrylic Roof Coating for Restoring Modified Bitumen and Smooth Built-Up Roofing Systems (Revised 05/2026)
  14. IIBEC, Interface (William A. Kirn, Rohm and Haas), ASTM D-6083 Standard Specification for Liquid Applied Acrylic Coating Used in Roofing: What It Says, What It Means, How It Came to Be (January 2001)
  15. BASF (acrylic resin maker), Raising the roof (coating standards) (September 26, 2018)
  16. Gaco (Amrize Building Envelope), Application Specification RC-A47-12-5: GacoFlex A47 Series Acrylic Roof Coating for Recoating Acrylic Roof Coating Systems (Revised 01/2024)
  17. Progressive Materials (PM Silicone), Recommended Design Specification 07545: Acrylic Roof Coating Restoration System over Modified Bitumen or Smooth Surface BUR
  18. Karnak Corporation, Roof Restoration System ASPHALT 405-501W: application guidelines
  19. Progressive Materials (PM Silicone), Recommended Design Specification 07545: Acrylic Roof Coating Restoration System over Metal Roof Panel (July 2025)
  20. Gaco (Amrize Building Envelope), Product Data Sheet (PDS): GacoFlex 127 Series Acrylic Roof Coating (Revised 07/2025)
  21. ICC Evaluation Service, ESR-4038: Polyglass Premium Grade Elastomeric Roof Coating Systems
  22. ICC Evaluation Service, ESR-3796: APOC asphalt emulsion, polyester fabric and liquid-applied roof coating systems
  23. Cool Roof Rating Council, Rated Products Directory: Henry AcryShield A500 White, 0620-0066
  24. Cool Roof Rating Council, Rated Products Directory: Sikalastic 515 AC, 0674-0046
  25. Cool Roof Rating Council, Rated Products Directory: Polyglass PG 700, 0616-0007
  26. Tremco Roofing and Building Maintenance, Solargard Restoration Acrylics brochure (2023)
  27. Miami-Dade County, Product Control Section, Notice of Acceptance 26-0121.02: Everest Systems Evercoat acrylic roof coatings (approved April 23, 2026)
  28. Gaco (Amrize Building Envelope), GacoFlex A47 product page
  29. ICC Evaluation Service, ESL-1479: Western Colloid ElastaHyde 790 AFC Fluid-Applied Roof Coating System

Updated October 2026.